AWS ER309Si Waea Kowiri tira MIG me te TIG Welding Rods Whakakii Waea

Whakaahuatanga Poto:

Ko te waea kowiri tira he nui te pai o te whakakii, he pai te mahi hangarau i roto i nga waahi katoa.E whakamahia nuitia ana i roto i te ahumahi: nga hanganga hangahanga, te waka, te miihini piriti, nga miihini maina, te rerewe, te paipa hinu, nga taputapu pehanga hau, nga taputapu hiko, me era atu.


Taipitopito Hua

Tohu Hua

Whakarōpū AWS:AWS 5.9

WHAKAMAHI:

Ko te waea kowiri tira he nui te pai o te whakakii, he pai te mahi hangarau i roto i nga waahi katoa.E whakamahia nuitia ana i roto i te ahumahi: te hanga hangahanga, te waka, te miihini piriti, nga miihini maina, te rerewe, te paipa hinu, nga taputapu pehanga hau, nga taputapu hiko, me era atu.

TAUIRA NO.& RAHI:

1. wheketere whakarato ratonga OEM.

2. Tauira : ER308 ER308L ER308LSi ER309 ER309L ER316 ER316L ER316LSi etc.

3. Rahi waea MIG: 0.8mm 0.9mm 1.0mm 1.2mm 1.6mm.

4.TIG waea rahi: 1.6mm 2.0mm 2.4mm 3.2mm 4.0mm.

WHAKATOKANGA:

Ka whakaratohia e matou nga momo momo waea whakarewa kowiri tira, tae atu ki te Mig waea whakapiri totoka, Tig rod waea whakapiri me te waea whakaahuru-arc, he kounga teitei katoa, ka hokona ki te ao katoa.

Engari mo te 308 me te 309, ka tukuna ano e matou te 304, 321, 347, 316L, 310, 2209, me 201. Me nga korero motuhake penei i te 318L, 904L, 2594, NiCrMo-3, Ni1.

KAKI:

Mig fehokotaki'anga waea tarapēke (spool and drum pack)

Taone: 0.8 - 2.0mm

Mōkī:1 kg/poka, 5 kg/poka, 15 kg/poka, 20 kg/poka, 100 kg/pahu, 200 kg/pahu

Tig rod fehokotaki waea tarapēke (ngongo kirihou)

Diane: 1.0 - 5.0mm

Mōkī: 5 kg/pack

Waea whakapiri pewa kua rukuhia

Diane: 2.5 - 5.0mm

Mōkī: 20kg / mōkihi, 25 kg / mōkihi

Ko nga kohinga koretake me te OEM e pai ana!

NGĀ HOTO MAU O TE WAWAU WHAI WHAI MAHI:

Tauira No.

C

Si

Mn

P

S

Cr

Ni

Mo

Cu

304

0.08

0.30-1.00

2.00

0.045

0.030

18.00-20.00

8.00-11.00

0.18

0.003

304L

0.03

0.30-1.00

2.00

0.045

0.030

18.00-20.00

8.00-12.00

ER307

0.04-0.14

0.30-0.65

4.30-4.75

0.030

0.030

19.50-22.00

8.00-10.70

0.5-1.5

0.75

ER308

0.08

0.30-0.65

4.30-4.75

0.030

0.030

19.50-22.00

9.00-11.00

0.75

0.75

ER308L

0.03

0.30-0.65

1.50-2.30

0.03

0.02

19.5-21.5

9.00-11.00

0.75

0.75

ER308LSi

0.03

0.65-1.00

1.60-2.40

0.03

0.02

19.5-21.5

9.0-11.0

0.75

0.75

ER309

0.12

0.30-0.65

1.00-2.50

0.03

0.03

24.0-25.0

12.0-14.0

0.75

0.75

ER309L

0.03

0.3-0.65

1.5-2.3

0.03

0.02

23.0-25.0

12.0-14.0

0.75

0.75

ER309LSi

0.03

0.65-1.0

1.6-2.4

0.03

0.02

23.0-25.0

12.0-14.0

0.75

0.75

ER316

0.08

0.3-0.65

1.0-2.5

0.03

0.03

18.00-12.00

11.0-14.0

2.0-3.0

0.75

ER316L

0.03

0.3-0.65

1.5-2.3

0.03

0.02

18.0-20.0

11.0-13.0

2.05-2.55

0.75

ER316LSi

0.03

0.65-1.0

1.6-2.4

0.03

0.02

18.0-20.0

11.0-13.0

2.05-2.55

0.75

ER310

0.08-0.15

0.3-0.65

1.0-2.5

0.03

0.03

25.0-28.0

20.0-22.5

0.75

0.75

ER347

0.08

0.3-0.65

1.0-2.5

0.03

0.03

19.0-21.5

9.0-11.0

0.75

0.75

ER317

0.08

0.3-0.65

1.0-2.5

0.03

0.01

18.5-20.5

13.0-15.0

3.0-4.0

0.75

ER321

0.08

0.3-0.65

1.5-2.5

0.03

0.01

18.5-20.5

9.0-10.5

0.75

0.75

NGA AHUATANGA MAHI O TE WAERE WELDING:

Tauira No.

Te kaha Rm(Mpa)

Te kaha tuku Rel, Rp0.2(Mpa) ranei

Te whakaroa

(%)

Tauira No.

Te kaha Rm(Mpa)

Te kaha tuku Rel, Rp0.2(Mpa) ranei

Te whakaroa

(%)

304

550

--

25

ER309LSi

510

320

25

304L

510

--

25

ER316

510

320

25

ER307

590

350

25

ER316L

510

320

25

ER308

550

350

25

ER316LSi

510

320

20

ER308L

510

320

25

ER310

550

350

25

ER308LSi

510

320

25

ER347

550

350

25

ER309

550

350

25

ER317

550

350

25

ER309L

510

320

25

ER321

550

350

25

TIG me MIG kowiri tira hangahanga waea fehokotaki'anga

YB5092-2005

AWS

Hanga matū %

C

Si

Mn

P

S

Cr

Ni

Mo

H08Cr20Ni9Mn7Si

ER307Si

0.075

0.78

6.7

0.022

0.01

19.8

8.8

H06Cr21Ni10

ER308

0.045

0.45

1.9

0.02

0.009

20.8

9.8

H0OCr21Ni10

ER308L

0.02

0.32

1.9

0.011

0.006

20

10.2

H06Cr21Ni10Si

ER308Si

0.045

0.85

1.5

0.022

0.01

20.8

9.8

H06Cr24Ni13

ER309

0.06

0.45

1.9

0.019

0.009

24.3

13.2

H06Cr24Ni13Si

ER309Si

0.06

0.79

1.95

0.019

0.009

24.7

13.2

H03Cr24Ni13

ER309L

0.02

0.42

1.8

0.02

0.01

24.8

13.2

H03Cr24Ni13Si

ER309LSi

0.018

0.8

1.7

0.02

0.01

23.5

13.5

H21Cr16Ni35

ER330

0.2

0.38

1.5

0.022

0.01

16.5

34.5

H06Cr19Ni12Mo2

ER316

0.04

0.4

1.9

0.02

0.01

19.5

11.8

2.3

H06Cr19Ni12Mo2Si

ER316Si

0.05

0.7

1.92

0.02

0.01

19.5

11.8

2.3

H03Cr19Ni12Mo2

ER316L

0.019

0.38

1.8

0.018

0.01

19.8

12.2

2.5

H03Cr19Ni12Mo2Si

ER316LSi

0.06

0.85

1.7

0.022

0.01

18.8

12.6

2.4

H03Cr17Ni14Mo3

ER317L

0.02

0.38

1.8

0.02

0.01

18.8

13.8

3.6

H08Cr19Ni12Mo2Nb

ER318

0.06

0.42

1.5

0.022

0.01

18.5

11.8

2.3

H07Cr20Ni34Mo2Cu3Nb

ER320

0.06

0.4

1

0.022

0.01

19.8

33.3

2.8

Nb0.7

H02Cr20Ni34Mo2Cu3Nb

ER320L

0.018

0.33

1.5

0.013

0.01

19.8

33.6

2.5

Nb0.35

H08Cr20Ni10Ti

ER321

0.06

0.45

1.5

0.022

0.01

20.8

9.8

Ti9xC-1.0

H08Cr21 Ni10Nb

ER347

0.055

0.48

1.8

0.021

0.008

20.8

9.8

Nb1xC-1.0

H12Cr26Ni21

ER310

0.09

0.5

1.66

0.02

0.01

25.5

20.5

H02Cr20Ni25Mo4Cu

ER385

0.02

0.3

1.5

0.018

0.01

20.2

24.8

4.8

Cu 1.80

H03Cr22Ni9Mo3N

ER2209

0.022

0.5

0.9

0.02

0.01

22.5

8.8

3.3

N0.08-0.20

H04Cr25Ni5Mo3Cu2N

ER2553

0.027

0.5

1

0.025

0.015

24.8

5.5

3.2

N0.1-0.25

H1 5Cr29Ni9

ER312

0.09

0.38

1.5

0.022

0.01

29.5

8.5

H03Cr24Ni13MoL

ER309L Mo

0.023

0.45

1.5

0.022

0.01

23.8

13.2

2.2

H05Cr17Ni4Cu4Nb

ER630

0.04

0.39

0.5

0.022

0.01

16.5

4.8

Cu;3 Nb;0.28

H08Cr26Ni5Mo2

ER453s

0.06

0.3

0.4

0.022

0.01

25.8

4.8

2.1

H08Cr21Ni10Mn6

0.06

0.35

5.5

0.022

0.01

20.8

9.8

H05Cr22Ni11Mn6Mo3VN

ER209

0.04

0.4

4.5

0.022

0.01

21.5

10.8

2.2

N;0.20 V;0.18

Wenzhou Tianyu Electronic Co., Ltd. i whakapumautia i te tau 2000. Kua mahi matou ki te hanga i nga hiko hiko, nga rakau raima, me nga taonga taapiri mo te neke atu i te 20 tau.

Ko o tatou hua matua ko nga irahiko kowiri tira, ko nga hiko waro, ko nga hiko o te waro, ko te iti o te koranu, ko te whakarewa i nga hiko, ko te nickel & cobalt koranu hiko, ko te rino ngawari me te iti o te koranu, ko nga waea kowiri tira, ko nga waea hiko, ko nga waea hiko. waea fehokotaki'i konumohe, whao i raro i te pewa.waea, nickel & cobalt koranu waea fehokotaki'anga, parahi fehokotaki'anga waea, TIG & MIG waea fehokotaki'anga, tungsten electrodes, waro gouging electrodes, me etahi atu taputapu fehokotaki'anga & pau.

 

Wenzhou Tianyu Electronic Co., Ltd. i whakapumautia i te tau 2000. Kua mahi matou ki te hanga i nga hiko hiko, nga rakau raima, me nga taonga taapiri mo te neke atu i te 20 tau.

Ko o tatou hua matua ko nga irahiko kowiri tira, ko nga hiko waro, ko nga hiko o te waro, ko te iti o te koranu, ko te whakarewa i nga hiko, ko te nickel & cobalt koranu hiko, ko te rino ngawari me te iti o te koranu, ko nga waea kowiri tira, ko nga waea hiko, ko nga waea hiko. waea fehokotaki'i konumohe, whao i raro i te pewa.waea, nickel & cobalt koranu waea fehokotaki'anga, parahi fehokotaki'anga waea, TIG & MIG waea fehokotaki'anga, tungsten electrodes, waro gouging electrodes, me etahi atu taputapu fehokotaki'anga & pau.


  • Tōmua:
  • Panuku: